Open Access
Table 5
The results of tensile test from base metals and full penetrate welds.
Sample number | Yield stress (MPa) | Ultimate stress (MPa) | Location of failure | Heat input (J/mm) |
---|---|---|---|---|
AISI 4340 base metal | 475 | 744 | – | – |
AISI 316L base metal | 190 | 515 | – | – |
4 | 210 | 543 | AISI 316L | 150 |
5 | 221 | 568 | weld/HAZ 316L | 192 |
6 | 178 | 198 | weld | 158 |
7 | 182 | 224 | weld | 158 |
8 | 235 | 590 | AISI 316L | 158 |
13 | 211 | 540 | AISI 316L | 158 |
14 | 225 | 580 | AISI 316L | 174 |
15 | 198 | 524 | weld/HAZ 316L | 190 |